Source: Chandrasekar Sundaravelu

Nov 2026 : Busbars and its Importance:

Busbars are key components in electric vehicle (EV) battery packs, providing electrical connections between individual cells to form modules and between modules to form the full pack. Busbar-to-busbar and busbar-to-cell terminal interconnections are critical to overall system performance, making their design and reliability of joint connections are of paramount importance. Any defects occurring in these interconnections severely affect joint integrity and result in a poor performance. [1] Suboptimal connections, characterized by a high electrical resistance or poor mechanical strength, can severely compromise the entire battery system. A high joint resistance leads to significant I2R (ohmic) losses, which manifests as waste heat and a reduction in the overall power output and energy efficiency of the battery pack [2].

Fig [1] An illustration of tab-to-tab and tab-to-busbar joints [3]

Material selection:

Typically, a pouch cell consists of two terminal tabs that protrude through seals to allow external connection. Copper (Cu) and aluminium (Al) are widely accepted tab (also busbar) materials for pouch cells and act as the negative and positive terminals, respectively.

The selection of busbar materials and geometries in battery modules represents a fundamental engineering optimization problem, primarily balanced between volumetric efficiency and gravimetric efficiency. While Copper exhibits superior intrinsic physical properties - such as lower electrical resistivity, higher thermal conductivity, and superior tensile strength - its application is penalized by high mass density. Conversely, Aluminium provides a superior conductivity-to- weight ratio, making it the preferred candidate for weight-sensitive applications like automotive electric vehicles. In this review we discuss Al Tab joining with Cu busbar.

Joining:

Dissimilar Al and Cu can be joined using Laser Beam Welding (LBW) with a major advantage of high throughput, Exceptional Process Speed, Non-Contact Execution, Localized Heat Delivery, Flexible Joint Geometry despite of high capital investment.

Al – Cu Laser Beam Welding (LBW) challenges :

Major challenges are, formation of the brittle intermetallic compounds (IMCs), Spatter, Cracks and Porosity.

Weld Joint Specification:

Porosity specifications for Aluminium-to-Copper (Al-Cu) busbar welding are tightly controlled because voids directly decrease the mechanical strength and increase the electrical contact resistance of the joint. The most common standard applied to EV laser welding is ISO 13919-2 (Electron and Laser-Beam Welded Joints). EV busbars almost always mandate Quality Level B [3]

Total projected area of porosity must not exceed 2% to 3% of the total weld area. Single larger pores are typically restricted to ≤ 0.2 × the joint thickness or a maximum of 0.3 mm to 0.5 mm.

Cracks & Micro-fissures: 0% Tolerance. Hot cracking in the Al-Cu Intermetallic Compound (IMC) zone is a critical failure.

IMC layer thickness Target <1.5 μm to 3 μm, this range ensures full metallurgical adhesion without introducing brittle mechanics. The Al-Cu intermetallic compounds behave highly resistive when exceeding a distinctive limit of 3-6 µm [4].

Defect formation mechanisms:

Porosity: T. Florian et al. studied the pore-forming mechanisms during laser beam welding of copper [5]

Bulging Pores: Melt Pool Sloshing & Capillary Instability:

•  They originate from a bulge at the rear keyhole wall.
•  An upward-directed melt flow interacts with an expanding keyhole to form the bulge.
•  The flow direction then reverses, generating high dynamic pressure.
•  This pressure constricts and detaches the bulge into a pore in less than 2milliseconds.
•  The pore is then quickly trapped by the immediate solidification line.

Fig [2] Formation of Bulging Pores [5]

Spiking Pores: Vapor Pressure Surge & Micro Vortices:

•  They occur following a rapid, locally limited increase in keyhole penetration depth
•  This rapid drilling process happens in less than 0.1 milliseconds.
•  The sudden protrusion induces a micro vortex in the melt flow.
•  The vortex pushes against the kink of the newly formed keyhole tip.
•  This detaches the tip, which is instantly frozen by the surrounding cold bulk material.

Fig [3] Formation of Spiking Pores [5]

Traveling Pores: Chaotic Evaporative Waves

•  They stem from chaotic, unstable waves ascending the rear wall of the keyhole.
•  Localized evaporation and heterogeneous vapor flows drive these waves upward.
•  Minor pores frequently pinch off from these dynamic regions at the temporal limit of the process (~0.05 ms).
•  These pores travel through the liquid melt pool.
•  They either escape entrapment by reabsorbing into the keyhole or get permanently trapped by the solidification front.

Fig [4] Formation of Traveling Pores [5]

Depression Pores: Geometric Disconnection & Hydrostatic Collapse

•  They are triggered by a substantial upward melt flow resulting in massive melt ejections.
•  This ejection significantly broadens the upper aperture of the keyhole.
•  The remaining un-ejected liquid metal reverses its direction.
•  It slams back down, exerting high dynamic pressure against the kink at the keyhole bottom.
•  This detaches a pore, which fails to reattach due to ongoing residual melt flow and lasing separation.

Fig [5] Depression of Traveling Pores [5]

IMC formation mechanisms:

Two distinct phenomena were observed by Tianzhu Sun et al. in their ring- shaped laser beam impact on dissimilar welding of Al-Cu thin sheet studies. Firstly, the upward migration of Cu from the bottom to the top of the molten pool, driven by the upward flow within the molten pool caused by the recoil pressure at the bottom of the keyhole; secondly, the mixing of Al and Cu, predominantly occurring in the upper region of the molten pool, facilitated by the vortices generated on the two sides of the molten pool due to the Marangoni force [Fig 6].

Fig [6] IMC formation mechanisms [6]

Key characteristics of Cu-Al IMCs [7]

Laser Beam shaping:

Laser beam shaping is defined as the spatial and temporal adjustment of the beam intensity distribution. Two broad families: Static Beam Shaping (SBS) and Dynamic Beam Shaping (DBS)

Static beam shaping (SBS)

SBS refers to modifying the spatial intensity distribution to a fixed and desired shape, that is static (no variation in time) during the entire welding process.

Core - Ring:

Inner core coaxial to a ring-shaped beam proved advantageous in improving weld quality. While the keyhole opening can be stimulated by the high- power density of the core beam, the ring-shaped beam with wider area and lower power-density controls the heat dissipation in and around the molten pool [Fig 7] and, thus, the cooling rate. [8]

Fig [7] Inner core coaxial to a ring-shaped beam [3] Fig [8] BSS 0 to 1 [12]

Tianzhu Sun et al [12] studied the effect of core ring beam shaping in Al Cu welding. Beam splitting system (BSS) was used for defining the power distribution between the core beam and ring beam [Fig 8], with BSS = 0 corresponding to the core-only beam and BSS = 1 referred to the ring-only beam.

Effect of concentric ring-core laser configuration on pores:

A concentric ring-core laser configuration eliminates these four types of pores by widening the vapor channel, stabilizing fluid flow, and ensuring a uniform distribution of metal vapor.

Bulging Pores: The outer ring beam spreads heat across a wider top surface, significantly widening the keyhole neck. Because the opening is held wide open, the surrounding melt cannot easily close in or constrict the wall, preventing the liquid bridges that trap bulges into pores.[10]

Spiking Pores: Spreading power out prevents all the energy from focusing into a single, erratic drilling point. This shared core-ring energy stabilizes the floor of the keyhole and suppresses extreme penetration fluctuations, eliminating sharp spikes and their accompanying micro-vortices [10]

Traveling Pores: The balanced core-ring distribution ensures uniform absorption and continuous, steady evaporation along the entire keyhole wall. This produces a highly homogeneous metal vapor distribution inside the channel, completely smoothing out the chaotic wall ripples that shed traveling pores [5]

Depression Pores: The ring beam effectively pre-heats and conditions the upper melt pool boundaries, smoothing out fluid velocity and reducing the surface tension spikes that lead to violent explosions. By suppressing large-scale spatter and melt ejections, it prevents the massive fluid back-flows that seal off the bottom of the weld. [5]

Effect of concentric ring-core laser configuration on IMC:

A coaxial core-ring laser system alters intermetallic compound (IMC) formation by optimizing the spatial power distribution to suppress the turbulent fluid forces that drive material mixing.

Mitigation of Recoil Pressure and Marangoni Vortices

•  The Unshaped Core-Only Problem (BSS = 0): A single focused core beam generates an extreme localized energy density. This triggers a massive vaporization-induced recoil pressure at the keyhole bottom, blasting copper upward from the lower sheet into the top aluminium layer Fig [9a]. Simultaneously, severe lateral thermal gradients trigger aggressive Marangoni vortices at the melt pool boundaries, trapping and violently blending the two liquid metals [9, 8].
•  The Ring-Core Solution: Transitioning to a dual-beam profile (such as the optimized 40% core / 60% ring split, (BSS = 0.6) drastically lowers the localized peak energy density. This directly weakens both the upward recoil jetting and the lateral Marangoni fluid flow, stabilizing the pool and halting the uncontrolled macro-mixing of Al and Cu [9,6].

2. Shifting IMC Phase and Morphology

•  Layer Thinning and Dispersion: Instead of forming the dense, heavily cracked, and thick IMC blocks seen in core-only welds, the core-ring profile alters the compound’s structure into thin, dispersed serial layers. This structural modification successfully redistributes local stress concentrations during subsequent mechanical loading [9].
•  Elimination of Free-State Phases: In core-dominated welds, the over- saturation of copper atoms produces massive networks of brittle, high- hardness throughout the upper fusion zone Fig [10]. The balanced ring-core laser restricts copper migration so successfully that these free-state brittle blocks disappear completely from the upper weld. Instead, the matrix solidifies into a ductile, primary eutectic phase from BSS of 0.6 and 1 [9].

Fig [9] Schematic of Al-Cu joint intermixing to evaluate the effect of dual-mode with (a) higher CP and lower RP and (b) lower CP and higher RP [3] Fig [10] EDS phase mapping showing the distribution of Al-Cu intermetallic compounds [9]

Summary:

Aluminium-copper (Al-Cu) joints are widely used in EV battery manufacturing for Cell-to-busbar connections. However, welding these dissimilar metals remains highly challenging due to the significant mismatches in their physical, thermal, and mechanical properties. Laser welding is the primary joining process for these connections in the automotive industry, yet producing defect-free joints remains a significant challenge. Laser beam shaping helps reduce these defects - such as spatter and porosity - by optimizing the weld pool geometry. Compared to conventional, core-only Gaussian beam welding, static beam shaping achieves superior mechanical strength and lower electrical contact resistance. Our work currently focuses on Al Cu joint quality improvement using various beam shaping techniques.

Author:
Reviewer:
Chandrasekar S
Dr. M Ramu
Jaguar Land Rover
Amrita University
csundara@jaguarlandrover.com
https://www.amrita.edu/faculty/m-ramu/

References

1. Ferreira, G.F.S et al. Busbar Interconnections in Electric Vehicle Batteries: A Review of Joining Technologies and Performance. Welding 2026
2. Choi, S et al, Tab-to-Busbar Interconnections in EV Battery Packs: An Introductory Review of Typical Welding Methods. Micromachines 2026
3. N. Kumar et al. Dual-mode laser beam welding of similar and dissimilar material tab-to-busbar for electric vehicle battery pack J. Adv. Join. Process.
4. Solchenbach T et al. Electrical performance of laser braze-welded aluminium-copper interconnects. J Manuf Process
5. T. Florian, K et al. Combining in situ synchrotron X-ray imaging and multiphysics simulation to reveal pore formation dynamics in laser welding of copper, International Journal of Machine Tools and Manufacture, Volume 204,2025
6. Wenkang Huang, et al. Investigation of metal mixing in laser keyhole welding of dissimilar metals, Materials & Design, Volume 195, 2020,109056,ISSN 0264-1275
7. P. Schmalen, et al. Composition and phases in laser welded Al-Cu joints by synchrotron x-ray microdiffraction, Procedia CIRP, Volume 74,2018, Pages 27-32
8. R. Al Botros, et al. Effect of static laser beam shaping on lateral and vertical gap bridging for welding of rectangular copper hairpin windings, 2024
9. Tianzhu Sun, et al. The impact of ring-shaped laser beam on dissimilar welding of Al-Cu thin sheets for battery tab-to-busbar connection: Microstructural, mechanical and electrical characteristics, Optics & Laser Technology, Volume 179,2024,111312
10. Chianese, G.et al. A multi-physics CFD study to investigate the impact of laser beam shaping on metal mixing and molten pool dynamics during laser welding of copper to steel for battery terminal-to-casing connections. Journal of Materials Processing Technology, 322, 118202